| Grade : | 42CrMo4 | |||||||
| Number: | 1.7225 | |||||||
| Standard: |
| |||||||
| Classification: | Alloy special steel | |||||||
| Equivalent grades: | Go here |
| C | Si | Mn | P | S | Cr | Mo |
| 0.38 - 0.45 | max 0.4 | 0.6 - 0.9 | max 0.025 | max 0.035 | 0.9 - 1.2 | 0.15 - 0.3 |
| Nominal diameter (mm): | to 16 | 16 - 40 | 40 - 100 | 100 - 160 | 160 - 250 | 250 - 330 | 330 - 660 |
| Rm - Tensile strength (MPa) (+QT) | 1100-1300 | 1000-1200 | 900-1100 | 800-950 | 750-900 | 700 | 600 |
| Nominal thickness (mm): | 0.3 - 3 |
| Rm - Tensile strength (MPa) (+A) | 620 |
| Rm - Tensile strength (MPa) (+AC) | 630 |
| Nominal thickness (mm): | to 8 | 8 - 20 | 20 - 50 | 50 - 80 |
| Rm - Tensile strength (MPa) (+QT) | 1100 | 1000 | 900 | 800 |
| Rm - Tensile strength (MPa) (+C) | 720 |
| Rm - Tensile strength (MPa) (+LC) | 670 |
| Nominal diameter(mm): or for flat products thickness: to 8; 8-20; 20-60; 60-100; 100-160; | to 16 | 16 - 40 | 40 - 100 | 100 - 160 | 160 - 330 | 330 - 660 |
|
Re - Upper yield strength or Rp0.2 - 0.2% proof strength (MPa) (+QT) | 900 | 750 | 650 | 500-550 | 460-500 | 390 |
| Nominal thickness(mm): | 0.3 - 3 |
| Rp0.2 0.2% proof strength (MPa) (+A) | 480 |
| KV - Impact energy (J) longitud., (+QT) | +20° 30-35 |
| KV - Impact energy (J) transverse, (+QT) | +20° 22 |
| Nominal thickness (mm): | 0.3 - 3 |
| A - Min. elongation Lo = 80 mm (%) (+A) | 15 |
| A - Min. elongation at fracture (%) transverse, (+QT) | 10-14 |
| A - Min. elongation at fracture (%) (+C) | 4 |
| A - Min. elongation at fracture (%) (+LC) | 6 |
| Nominal thickness (mm): | to 16 | 16 - 40 | 40 - 100 | 100 - 160 | 160 - 250 |
| A - Min. elongation Lo = 5,65 √ So (%) (+QT), round products | 10 | 11 | 12 | 13 | 14 |
| Nominal diameter (mm): or for flat products thickness: to 8; 8-20; 20-60; 60-100; 100-160; | to 16 | 16 - 40 | 40 - 100 | 100 - 160 | 160 - 250 |
| Z - Reduction in cross section on fracture (%) (+QT) | 40 | 45 | 50 | 50 | 55 |
| Z - Reduction in cross section on fracture (%) (+AC) | 57 |
| Brinell hardness (HBW): (+S) | 255 |
| Brinell hardness (HBW): (+A) | 241 |
| Vickers hardness ( HV): (+A) | 195 |
| Vickers hardness ( HV): (+QT) | 340 - 490 |
| Weldability: Bad weldability due to the high crack danger.
Hardenability: Medium-good hardenability, suitable for hot purposes till a temperature of 500 C. It can be hardened in oil. |
| USA - | Germany DIN,WNr | Japan JIS | France AFNOR | England BS | Italy UNI | Spain UNE | China GB | Sweden SS | Finland SFS | Russia GOST | Inter ISO | ||||||||||||||||
|
|
|
|
|
|
|
|
|
|
|
|
| ReH | Minimum yield strength / Mindestwert der oberen Streckgrenze / Limite d�elasticite minimale |
| Rm | Tensile strength / Zugfestigkeit / Resistance a la traction |
| A | Minimum elongation / Mindestwert der Bruchdehnung / Allongement minimal |
| J | Notch impact test / Kerbschlagbiegeversuch / Essai de flexion par choc |
| +A | Soft annealed |
| +AC | Annealed to achieve spheroidization of the carbides |
| +AR | As rolled |
| +AT | Solution annealed |
| +C | Cold drawn / hard |
| +CR | Cold rolled |
| +FP | Treated to ferrite-pearlite structure and hardness range |
| +I | Isothermal annealing |
| +LC | Cold drawn / soft |
| +M | Thermo mechanical rolling |
| +N | Normalized |
| +NT | Normalized and tempered |
| +P | Precipitation hardened |
| +PE | Peeled |
| +QA | Air quenched and tempered |
| +QL | Liquid quenched and tempered |
| +QT | Quenched and tempered |
| +S | Treated to improve shearability |
| +SH | As rolled and turned |
| +SR | Cold drawn and stress relieved |
| +T | Tempered |
| +TH | Treated to hardness range |
| +WW | Warm worked |
| +U | Untreated |
| The entire risk as to use of these content is assumed by you the user |